Blend into repaired panel - 35 Line Non VOC 35 1. Cleaning step Clean carefully with cleaner 70-10 Use wipe on wipe off method 2. Cleaning Tack cloth the area to be painted 3. Basecoat 35- Basecoat 100% 60- Diluter 50% Temperature chart 4. Basecoat Spray gun HVLP 1.3, pressure 0.8 to 1.5 bar Spray first coat over filler patch Keep the patch as small as possible Flash off until matt 5. Flash off Flash of the basecoat until matt 6. Tack cloth Tack cloth clean the surrounding area, to remove overspray 7. Basecoat Apply second coat over fillerpatch, by fading out the basecoat Blend the basecoat until invisible repair 8. Flash off Flash off the basecoat until matt 9. Mist coat Apply a mist coat over the repaired area Spray gun distance is 30 cm Flash off Panel is now ready for clearcoat Repair Steps Lakier bazowy/ nawierzchniowy Zacznij pracę z baslac już dziś - to się po prostu opłaca. Skontaktuj się z nami Skontaktuj się z lokalnym partnerem baslac już dziś i pracuj efektywniej. Znajdź dystrybutora w swojej okolicy