原子灰施工工艺 - 金属件- CV 30系列

30CV

TST 13 (1).png

1. Preparation for putty

  • Clean carefully with  70-10
  • Sand the damage with P150
  • For small repairs, keep the sanding area as small as possible
TST 13 (2).png

2. Mixing ratio of putty

  • 12-20 Putty 100%
  • 56-20 Hardener 3% by weight
  • Mix until uniform color

Dry properties

  • 20 min at 20°C
  • 4 min short wave
TST 13 (4).png

3. Sanding guide

  • Use of sanding guide, highlights surface imperfections and possible sand scratches prior to finish with abrasives
TST 13 (5).png

4. Sanding steps

  • Hand block the putty first with P 150/240
TST 13 (3).png

5. Sanding steps

  • Fine sand the area with orbit machine: P 240
  • Surround area with P 320
TST 13 (6).png

6. Cleaning

  • Clean carefully with 70-10
  • Use wipe on, wipe off method (2 cloths)
Repair Steps

立即开始使用百事利。这是有道理的。