中涂施工 - 铝材

VOC 45 Line 45系列VOC

TST 61 (1).png

1. Masking 遮蔽

  • Mask the repair area 遮蔽修补区域
  • make sure to mask with soft edges, hard edges will leave marks in basecoat.

    确保使用软边进行遮蔽,硬边会在底漆上留下痕迹。

  • Clean with 70-10 使用70-10清洁
TST 61 (8).png

2. Mixing ratio 调配比例

  • Washprimer 27-10 磷化底漆 100%
  • Hardener 57-10 固化剂 50%
  • Reducer 60- 稀释剂 30%
TST 61 (2).png

3. Primer application 底漆施工

  • Spray gun HVLP 1.3, 2 bar HVLP喷枪1.3口径,2.0巴
  • Apply 1 coat over the bare aluminium. 在裸露的铝材上喷涂1层

 

Application 应用:

  • 1 coat (see 27-10 TDS) 喷涂1层(见27-10 TDS)

 

Flash off 闪干:

  • 10 min at 20° /  20°,10分钟
TST 61 (10).png

4. Product preparation 产品准备

  • Prepare undercoat accoridng to color 20-24 根据颜色20-24准备底漆
  • To obtain different colors, fillers can be mixed 为了获得不同的颜色,可以混合中涂
TST 61 (9).png

5. Mixing ratio 调配比例

TST 61 (3).png

6. Application of filler 中涂施工

  • Spray 2 wet coats on repair 喷涂2湿层
  • Stay with second coat in the patern of first coat as shown on the picture

    保持第二遍喷涂的走向与第一遍一致,如图所示。

Dry 干燥

  • 8 min short wave 短波8分钟
  • 3 hours at 20°C / 20°C,3小时
TST 61 (4).png

7. Sanding guide 打磨指南

  • Use of sanding guide, highligts surface imperfections and possible sand scratsches prior to finish with abrasives.

    使用打磨指南,可以在使用磨料完成之前突出表面缺陷和可能存在的打磨划痕。

TST 61 (5).png

8. Sanding steps 打磨步骤

  • Fine sand area with orbit machine P 320 用P320砂纸配合机器细磨区域
  • Surround area with P 400/ P 500 用P 400/ P 500砂纸打磨周围区域
TST 61 (6).png

9. Sanding steps 打磨步骤

  • Fine sand area with 3mm orbit machine and P 320

    用3mm 偏心打磨机盘和 P320 砂纸进行精细打磨

  • finish with P 400/ P 500  

    用P400 / P500 完成打磨

  • Blend in area P1000/2000 用P100 0/2000砂纸打磨过渡区域
TST 61 (7).png

10. Cleaning清洁:

  • Clean carefully with 70-45  用70-45仔细清洁
Repair Steps

立即开始使用百事利。这是有道理的。

立即联系您当地的百事利经销商,开始更智能地工作。